Extrusion & Post 6 görüntüleme

Dimensional Fluctuation of High-Density Polyethylene Extruded Products

Sorun Belirtisi
The outer diameter, wall thickness, or width of the extruded product fluctuates periodically or randomly in the longitudinal direction. Dimensional fluctuation affects the fitting accuracy and service performance of the product and is common in pipe and profile extrusion.
Neden Analizi
(1)The screw rotation speed is unstable, and the output fluctuates (2)The haul-off speed is unstable and does not match the extrusion speed (3)The barrel temperature fluctuates greatly, and the melt viscosity changes (4)The raw material feeding is uneven, and the material discharge fluctuates (5)The cooling water temperature or flow fluctuates
Çözüm
(1)Check the extruder drive system to stabilize the screw rotation speed (2)Check the haul-off machine speed control system to ensure stable haul-off speed (3)Stabilize the barrel temperature, with the fluctuation controlled within ±3°C (180-260°C range) (4)Check the hopper discharge to ensure continuous and uniform feeding (5)Stabilize the cooling water temperature and flow, and add a constant temperature device when necessary
Temel Çıkarım
Dimensional fluctuation is caused by unstable extrusion or haul-off, and all process parameters need to be systematically stabilized.
dimensional fluctuationscrew rotation speedhaul-off speedtemperature stabilityuniform feeding