Material Analysis
5 görüntüleme
Insufficient Strength of High-Density Polyethylene Film
Sorun Belirtisi
The tensile strength or tear strength of the film is lower than the standard requirement, and it is easily damaged in use.
Insufficient strength affects the protective function of the film and is especially critical in heavy-duty packaging films and industrial films.
Neden Analizi
(1)The raw material MFR is high, the molecular weight is low, and the strength is poor
(2)The melt temperature is too high, and the material degrades
(3)The blow-up ratio or draw ratio is improper, and the molecular orientation is unreasonable
(4)The film thickness is insufficient
(5)The regrind ratio in the raw material is too high
Çözüm
(1)Select a grade with a lower MFR to increase the molecular weight
(2)Control the extrusion temperature within the 180-260°C range to avoid overheating degradation
(3)Optimize the blow-up ratio (2-4) and draw ratio (3-6) to balance the longitudinal and transverse strength
(4)Check and adjust the film thickness to the standard value
(5)Control the regrind ratio to no more than 10%
Temel Çıkarım
Insufficient film strength is caused by improper material selection or process parameters, and needs to be optimized from raw materials, temperature, and blow-up ratio.