Extrusion & Post 5 görüntüleme

Die marks/lines appearing on linear low-density polyethylene extruded products (variant: strengthened measures)

Sorun Belirtisi
Continuous lines or marks appear on the extrudate surface along the extrusion direction at fixed positions. Die marks affect product appearance and are especially obvious in transparent products and films. Especially, additional attention is needed on top of the original basis; this problem is more prominent and requires focused attention.
Neden Analizi
(1) The die inner wall has scratches or damage (2) Impurities or carbides accumulate inside the die (3) Unreasonable die flow channel design with stagnation zones (4) The die joint is uneven (5) The breaker plate or screen is damaged, allowing impurities to pass through (6) On top of the original basis, additional attention is needed as process parameter fluctuations or equipment condition changes aggravate this problem
Çözüm
(1) Disassemble the mold and check the die inner wall; scratches need to be ground and polished for repair (2) Clean impurities and carbides inside the die, using copper tools to avoid damage (3) Optimize die flow channel design to eliminate stagnation dead zones (4) Grind the die joint flat to ensure no steps (5) Replace the breaker plate and screen, replacing regularly to prevent damage (6) And strengthen process monitoring; on top of the original basis, additional attention is needed to pay special attention to parameter stability
Temel Çıkarım
Die marks are caused by die inner wall damage or impurities; the die condition needs to be regularly cleaned and inspected. In different production scenarios, targeted preventive measures need to be taken.
die marksdie scratchesimpurity cleaningflow channel designscreen