Rough inner and outer walls of linear low-density polyethylene pipes

Sorun Belirtisi
The inner or outer wall surface of the pipe is rough, with visible streaks or particles. Rough pipe walls increase fluid resistance and affect conveying efficiency, and may affect hygiene performance in water supply pipes.
Neden Analizi
(1) Die or mandrel temperature is on the low side, and the melt surface is rough (2) Die or mandrel surface finish is insufficient (3) The sizing sleeve is worn or has a rough surface (4) Melt temperature is on the low side and fluidity is poor (5) Compressed air has high water content, affecting the inner wall
Çözüm
(1) Appropriately increase die and mandrel temperature to the higher value within the 190-250°C range (2) Polish the die and mandrel to Ra≤0.2μm, with chrome plating treatment (3) Check the sizing sleeve; replace if worn or rough (4) Appropriately increase barrel temperature to a reasonable value within the 190-250°C range (5) Add a drying and filtering device to the compressed air
Temel Çıkarım
Rough pipe walls are caused by low mold temperature or poor surface condition and need to be solved from temperature control and mold maintenance.