Metallocene linear low density polyethylene film cooling line height instability(Variant: Mass Production Scenario)

Sorun Belirtisi
The cooling line (frost line) height of the blown film fluctuates greatly, and film thickness and quality are unstable. The cooling line height reflects the stability of cooling conditions and directly affects film performance.In particular, during continuous mass production, this problem is more prominent and requires key attention.
Neden Analizi
(1) Air ring air volume or air speed unstable\ (2) Extrusion temperature fluctuates\ (3) Ambient airflow interference\ (4) Screw speed fluctuates\ (5) Cooling air temperature fluctuates\ (6) In continuous mass production, process parameter fluctuations or equipment status changes aggravate this problem
Çözüm
(1) Check the air ring fan and valves, ensure stable air volume\ (2) Stabilize the extrusion temperature, fluctuation controlled within ±3°C (190-260°C range)\ (3) Install wind shields or isolation curtains to reduce ambient airflow interference\ (4) Stabilize the screw speed\ (5) Use constant-temperature cooling air to reduce temperature fluctuations\ (6) And establish standardized work instructions, paying special attention to parameter stability in continuous mass production
Temel Çıkarım
Cooling line instability is caused by fluctuations in cooling or extrusion conditions, requiring stabilization of air ring parameters and environmental conditions.Targeted preventive measures need to be taken in different production scenarios.