Extrusion & Post
5 görüntüleme
Uneven wall thickness of polyolefin plastomer extruded pipes (Variant: strengthened measures)
Sorun Belirtisi
The wall thickness of the pipe is uneven in the circumferential direction, showing eccentric wall phenomenon.
Uneven wall thickness affects the pressure resistance of the pipe; the thin-walled side ruptures first under pressure, seriously affecting the safety of pipe use.
Especially on the original basis, additional attention is needed, and this problem is more prominent and requires key attention.
Neden Analizi
(1) Die and mandrel not concentric, gap uneven
(2) Melt temperature uneven, large circumferential temperature difference at the die
(3) Extruder output uneven, melt pressure fluctuates
(4) Haul-off speed unstable or haul-off center not concentric with the die
(5) Pipe sizing sleeve worn or improperly installed
(6) On the original basis, additional attention is needed: process parameter fluctuations or equipment state changes aggravate this problem
Çözüm
(1) Adjust the concentricity of die and mandrel, circumferential gap error not exceeding ±0.05mm
(2) Check die heating ring distribution, ensure circumferential temperature difference not exceeding ±3°C (180-230°C range)
(3) Check extruder plasticizing stability to ensure uniform output
(4) Adjust the center line of the haul-off device to align with the die center
(5) Check the sizing sleeve, replace if severely worn, ensure concentric installation
(6) And strengthen process monitoring; on the original basis, additional attention is needed, paying special attention to parameter stability
Temel Çıkarım
Uneven wall thickness is caused by uneven die gap or uneven temperature, and needs to be solved from mold accuracy and temperature uniformity.
Targeted preventive measures need to be taken in different production scenarios.