Extrusion & Post 12 görüntüleme

Poor blending stability of polyolefin plastomer POP and PE

Sorun Belirtisi
Delamination or uneven dispersion occurs when POP and PE are blended and extruded, and the mechanical properties and appearance of the product are uneven. Poor blending stability affects the consistency of product performance.
Neden Analizi
(1)The compatibility of POP and PE is limited, which is more obvious when the octene content differs greatly (2)The mixing is insufficient and the POP and PE particles are not uniformly mixed (3)The screw mixing capacity is insufficient (4)The extrusion temperature is improper, and the large melt viscosity difference makes dispersion difficult (5)The raw material particle size differs greatly
Çözüm
(1)Premix POP and PE before adding to the hopper, using a mixer for 5-10min (2)Select POP and PE grades with good compatibility (3)Add mixing elements to the screw design (4)Adjust the extrusion temperature so that the viscosities of the two materials are close (5)Add a compatibilizer (such as a block copolymer) when necessary
Temel Çıkarım
Blending stability needs to be improved from three aspects: mixing, screw design, and material matching.