Low-temperature brittleness problem of homopolymer polypropylene PP products

Sorun Belirtisi
PP (especially homo-PP) products become brittle when used below 0°C, with impact strength dropping sharply. Low-temperature brittleness is an inherent defect of homo-PP, limiting its application in cold environments.
Neden Analizi
(1) Homo-PP glass transition temperature is about 0°C; below this temperature impact strength drops sharply (2) High crystallinity of homo-PP, molecular chain segment movement restricted (3) Thin product walls or presence of notches, easy low-temperature failure (4) Processing internal stress aggravates low-temperature brittleness (5) Low-temperature resistant modified material not used
Çözüm
(1) For low-temperature use environments, PP COPO (block copolymer) should be selected to replace PP HOMO (2) Add elastomer toughening (e.g., EPDM, POE 5-20%) (3) Product design avoids sharp corners and notches (4) Increase mold temperature to the higher value within the 40-90°C range to reduce internal stress (5) Anneal the product after demolding to eliminate internal stress
Temel Çıkarım
PP low-temperature brittleness can be improved by selecting copolymer grades and adding toughening agents.