Material Drying 5 görüntüleme

Degradation of PBT due to excessive pre-drying

Sorun Belirtisi
PBT particles turn yellow and IV decreases when the drying temperature is too high or the time is too long.
Neden Analizi
When the drying temperature exceeds 130°C or the time exceeds 8h, PBT undergoes thermal oxidative degradation, especially when containing oxidative catalysts.
Çözüm
Strict drying temperature of 120°C/4-6h; use timing and temperature control protection; first in first out for materials in the drying hopper.
Temel Çıkarım
Over-drying of PBT is equally harmful.
PBTover-dryingdegradationdrying temperature