Injection Molding 12 görüntüleme

Insufficient Filling in PC '2079851475616104452

Sorun Belirtisi
The cavity of large PC products is not completely filled.
Neden Analizi
The melt viscosity of PC is high and sensitive to temperature; the injection pressure is insufficient; the gate and runner resistance is large; the mold temperature is low.
Çözüm
Increase the melt temperature to 290-310°C; increase the injection pressure; enlarge the gate and runner; mold temperature 90-120°C.
Temel Çıkarım
The high viscosity of PC is the main cause of short shot due to poor fluidity.