Injection Molding 12 görüntüleme

Uneven crystallization white haze of PET injection products

Sorun Belirtisi
White opaque areas appear locally on PET products, in obvious contrast with transparent areas.
Neden Analizi
Improper mold temperature control; local overcooling causes rapid PET crystallization forming spherulites; when mold temperature below 120°C, crystallization incomplete.
Çözüm
Increase mold temperature to 130-150°C, use a mold temperature controller for precise temperature control, optimize cooling water channels for uniform mold surface temperature.
Temel Çıkarım
PET crystallization behavior is very sensitive to mold temperature; uniform mold temperature is key.
PETuneven crystallizationwhite hazemold temperaturespherulite