Thermoforming 5 görüntüleme

Brittleness of PET sheet thermoformed products

Sorun Belirtisi
PET thermoformed food trays are brittle, break when bent, and have poor toughness.
Neden Analizi
Excessive crystallization during sheet heating (staying too long in the crystallization temperature zone); improper forming temperature; sheet IV is on the low side with too much recycled material.
Çözüm
Heat quickly to shorten the stay in the crystallization temperature zone; forming temperature 100-120°C; use sheet with IV≥0.70; fully dry before forming.
Temel Çıkarım
The brittleness of PET thermoformed products is related to excessive crystallization and material degradation.
PET'2079851475616104458brittlenessexcessive crystallizationIV value