Material Analysis 13 مشاهدة

Balance Between Vent Depth and Flash of PEEK

ظاهرة المشكلة
[Problem Phenomenon] Trapped-air burning and flash at the vents coexist on PEEK products, and deepening the vent grooves causes overflow
تحليل الأسباب
PEEK melt has low viscosity and easily overflows the edge, so the vent groove depth must be controlled within the precise range of 0.02-0.025mm; too shallow causes trapped-air burning, too deep causes flash
الحل
Precision-machine the vent groove depth at 0.02-0.025mm and clean it regularly; for trapped-air areas, prioritize optimizing the gate and injection speed profile; for flash, check the clamping and parting line fit
الخلاصة الأساسية
PEEK venting is 0.02mm-level fine work — depth precision is more important than deepening; after confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence
vent groove flash trapped air burnt