Injection Molding 8 مشاهدة

PET mold temperature 70-80℃

ظاهرة المشكلة
PET engineering injection molded parts warp and deform, or their heat resistance fails to meet the standard due to insufficient crystallization
تحليل الأسباب
PET injection mold temperature affects the crystallinity: low mold temperature leads to insufficient crystallization, poor product heat resistance, and post-crystallization deformation; an injection mold temperature of 70-80℃ combined with a cooling mold temperature of 40-50℃ can balance crystallization and cycle
الحل
①Mold temperature 70-80℃ in the injection stage; ②mold temperature 40-50℃ in the cooling stage; ③for products with high heat resistance requirements, ensure sufficient crystallinity; after adjustment, take consecutive samples to verify the effect, and resume mass production only after confirming stability
الخلاصة الأساسية
PET mold temperature is managed in stages; high temperature in injection ensures crystallization and low temperature in cooling ensures the cycle, and the two-stage combination is the standard practice for engineering parts; after confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence