Material Drying 5 مشاهدة

PET bottle-grade drying temperature

ظاهرة المشكلة
Bottle-grade PET is dried at 150℃ for 8 hours, and the chip IV value drops significantly with the preform body turning yellow
تحليل الأسباب
Bottle-grade PET drying temperature should be 165-175℃ to ensure crystallization and dehydration efficiency; when the temperature is too low, the drying time is forced to be extended, which instead aggravates thermal oxidation, and IV loss and yellowing follow
الحل
Bottle-grade PET is dried at 165-175℃ for 4-6 hours, crystallizing first and then drying; compensating for insufficient drying by extending the time is inferior to ensuring the temperature; after adjustment, take consecutive samples to verify the effect, and resume mass production only after confirming stability
الخلاصة الأساسية
Bottle-grade drying is a high-temperature short-time route, and low-temperature long-time instead harms the material; after confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence; include this case in the defect archive as a troubleshooting reference for subsequent similar problems