Material Drying
5 مشاهدة
PLA insufficient drying and hydrolysis
ظاهرة المشكلة
PLA products show bubbles and silver streaks with reduced strength, which improves after drying.
تحليل الأسباب
PLA easily absorbs moisture from the environment; moisture triggers hydrolysis, breaking ester bonds and reducing molecular weight; hydrolysis simultaneously produces apparent defects such as bubbles and silver streaks and deterioration of mechanical properties.
الحل
① Dehumidify and dry at 60~80℃ for more than 4 hours before processing; ② reduce moisture content to below 0.02%; ③ store sealed and open as needed; ④ shorten exposure time in humid environments.
الخلاصة الأساسية
PLA moisture sensitivity runs through the entire storage and processing process; hydrolysis is irreversible, and drying is the only means to protect molecular weight.; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence