Production & Quality 8 مشاهدة

Performance decay of EAA after repeated processing

ظاهرة المشكلة
After 3-4 times of recycling and reprocessing, the tensile strength of EAA decreases by 25-30%
تحليل الأسباب
Molecular chains break and degrade under repeated high-temperature shear; antioxidants are exhausted in multiple processing; cumulative effect of thermo-mechanical degradation
الحل
1) The proportion of recycled material should not exceed 20-30%; 2) Supplement 0.1-0.2wt% antioxidant in each re-extrusion; 3) Lower the processing temperature by 5-10°C; 4) Reduce the screw speed to reduce shear
الخلاصة الأساسية
Performance decay after multiple processing is caused by thermo-mechanical degradation; limiting recycled material and supplementing antioxidants are the key
EAA recycling performance decay antioxidant supplementation thermal degradation shear degradation