Injection Molding
5 مشاهدة
EVOH injection gate freezes too early
ظاهرة المشكلة
EVOH injection product gate freezes within 0.5-1s during the holding stage, holding pressure cannot be transmitted, product shrinkage severe
تحليل الأسباب
Gate size too small, diameter <1mm causing rapid freezing; injection temperature too low; mold temperature too low accelerating gate cooling
الحل
1) Increase gate diameter to 1.5-2mm; 2) Increase injection temperature to 190-230°C; 3) Increase mold temperature to 40-50°C to delay gate freezing; 4) Holding pressure stepwise decay rather than sudden release
الخلاصة الأساسية
Premature gate freezing is caused by small gate and low temperature; enlarging the gate and increasing temperature are fundamental measures