Injection Molding 5 مشاهدة

EVOH injection molded product ejector whitening

ظاهرة المشكلة
White marks (ejector whitening) appear at ejector pin positions on EVOH injection molded products, affecting appearance
تحليل الأسباب
Ejector pin force too large causing local compression deformation whitening; insufficient cooling time with the product ejected before full solidification; ejector pin area too small with stress concentration
الحل
1) Extend cooling time so the product is ejected after full solidification; 2) Increase ejector pin area using ejector plate instead of small ejector pins; 3) Reduce ejection speed to reduce impact; 4) Increase draft angle to reduce ejection force
الخلاصة الأساسية
Ejector whitening is caused by excessive ejection force and insufficient cooling; increasing ejector pin area and extending cooling time are key
EVOH injection ejector whitening ejector pin area cooling time draft angle