Extrusion & Post 12 مشاهدة

Delamination of PVA blended with incompatible resin

ظاهرة المشكلة
PVA blended with polar resins such as PA/ABS, extrudate completely delaminated, mechanical properties extremely poor
تحليل الأسباب
PVA and polar resin have large polarity difference, compatibility zero, interfacial adhesion extremely low, no compatibilizer used
الحل
1) Use PVA grafted compatibilizer PVA-g-MAH 2-5wt%; 2) Add epoxy-type compatibilizer 1-2wt%; 3) PVA addition <10wt% to keep the other resin as continuous phase; 4) Twin-screw high-shear blending to disperse PVA <0.3μm
الخلاصة الأساسية
Blends with large polarity difference need reactive compatibilizer to form chemical bonding at the interface to solve
PVA blend delamination polarity difference PVA-g-MAH reactive compatibilization interfacial bonding