Injection Molding 7 مشاهدة

Glass fiber reinforced plastic severe floating fiber

ظاهرة المشكلة
Glass fiber reinforced injection molded product surface has exposed glass fiber, rough and prickly to hand
تحليل الأسباب
Poor interfacial bonding between glass fiber and matrix pushes to surface, floating fiber phenomenon; injection speed too fast, glass fiber oriented at surface
الحل
1) Treat glass fiber with silane coupling agent KH-570 0.5-1wt% to improve interface; 2) add matrix-g-MAH 2-3wt% to strengthen interface and promote encapsulation; 3) reduce injection speed to reduce floating fiber; 4) mold temperature 50-60°C to improve surface encapsulation; 5) glass fiber length 0.5-1mm to reduce floating fiber
الخلاصة الأساسية
Floating fiber is caused by poor interface and injection orientation; coupling agent and reduced injection speed are key
glass fiber floating fibercoupling agentMAH compatibilizerinjection speedglass fiber length