Extrusion & Post
6 مشاهدة
Poor printability of linear low-density polyethylene film
ظاهرة المشكلة
Printing ink adhesion on the film surface is poor, and printed patterns fall off or are blurred.
Poor printability affects product appearance and affects product quality in printed packaging film.
تحليل الأسباب
(1) Linear low-density polyethylene has low surface energy (<32dyn/cm), and ink wettability is poor
(2) Film surface treatment is insufficient (corona treatment is not enough)
(3) There are exudates on the film surface (migration of slip agents and antiblocking agents)
(4) The ink does not match the film
(5) Printing environment humidity is improper
الحل
(1) Perform corona treatment to increase film surface tension to 38-42dyn/cm
(2) Control corona treatment power and treatment time to ensure uniform treatment
(3) Control additive dosage to avoid excessive migration
(4) Select ink types that match the film
(5) Control printing environment humidity at 50-60%
الخلاصة الأساسية
Poor printability is caused by low surface energy and needs to be improved by increasing surface tension through corona treatment to improve ink adhesion.
هل كان هذا مفيدًا؟
0 شخص وجدوا هذا مفيدًا
شكرًا لك على ملاحظاتك!