Extrusion & Post 7 مشاهدة

Metallocene linear low density polyethylene blown film uneven thickness(Variant: Startup Commissioning Scenario)

ظاهرة المشكلة
The film thickness fluctuates greatly in the circumferential or longitudinal direction, with thickness deviation exceeding ±10%. Uneven thickness affects film mechanical properties and service performance, and may cause tracking deviation or film breakage on automatic packaging machines.In particular, during new machine commissioning or the initial startup period, this problem is more prominent and requires key attention.
تحليل الأسباب
(1) Die gap is uneven\ (2) Die circumferential temperature is uneven\ (3) Air ring cooling is uneven\ (4) Extrusion output fluctuates\ (5) Haul-off speed is unstable\ (6) During new machine commissioning or the initial startup period, process parameter fluctuations or equipment status changes aggravate this problem
الحل
(1) Adjust the die gap, circumferential error not exceeding ±0.01mm\ (2) Check the die heater bands, ensure circumferential temperature difference does not exceed ±3°C (190-260°C range)\ (3) Check the air ring, ensure uniform air outlet, clean the air ring regularly\ (4) Stabilize the extruder screw speed and temperature\ (5) Stabilize the haul-off speed, use a high-precision haul-off control system\ (6) And do well in parameter recording and archiving, paying special attention to parameter stability during new machine commissioning or the initial startup period
الخلاصة الأساسية
Film thickness unevenness is caused by die gap, temperature or cooling unevenness, and needs to be solved from mold precision and process stability.Targeted preventive measures need to be taken in different production scenarios.
film thicknessdie gaptemperature uniformityair ring coolinghaul-off stability

هل كان هذا مفيدًا؟

0 شخص وجدوا هذا مفيدًا