Metallocene linear low density polyethylene MLLDPE excessive gel/gel particles
ظاهرة المشكلة
There are many gel particles and gel granules in the MLLDPE film, affecting the film appearance and mechanical properties.
The gel particle problem is particularly prominent in transparent films, reducing the product grade.
تحليل الأسباب
(1) MLLDPE has a narrow processing temperature window, and is not fully plasticized at low temperature\
(2) The barrel temperature is too low, and the high molecular weight fraction is not melted\
(3) The screw mixing section design is insufficient to fully plasticize MLLDPE\
(4) The raw material itself contains gel\
(5) The filter screen mesh count is too low
الحل
(1) Increase barrel temperature to 240-260°C, ensure full plasticization\
(2) Optimize the screw mixing section design\
(3) Increase the filter screen mesh count to 100-150 mesh\
(4) Select MLLDPE grades with few gel particles\
(5) Regularly clean the screw and die