Processing Machinery 6 مشاهدة

Excessive gels/gel particles in general-purpose polyethylene extruded products

ظاهرة المشكلة
Transparent or translucent gel particles (gel particles) are visible in the extruded film or product, affecting the appearance and transparency of the product. Gels are resin particles that are not fully plasticized or crosslinked.
تحليل الأسباب
(1)The high molecular weight components in the raw material are not fully plasticized (2)The barrel temperature is low, and part of the resin is not completely melted (3)The screw mixing effect is insufficient (4)The raw material contains crosslinked or oxidized gels (5)The filter screen mesh is not enough, and the gels are not intercepted
الحل
(1)Appropriately raise the barrel temperature to the higher value within the range of 160-260°C (2)Optimize the screw design and add mixing elements (3)Increase the filter screen mesh to 80-120 mesh (4)Select high-quality raw materials with low gel content (5)Check whether crosslinked materials are mixed into the regrind
الخلاصة الأساسية
Gels are caused by insufficient plasticization or raw material quality problems, and need to be solved from temperature control, screw design, and raw material selection.
gel gel particle plasticizing temperature screw mixing filter screen mesh