Excessive gel/gel particles in polyolefin plastomer extruded products

ظاهرة المشكلة
Transparent or translucent gel particles (gel particles) are visible in the extruded film or product, affecting the appearance and transparency of the product. Gel is resin particles that are not fully plasticized or cross-linked.
تحليل الأسباب
(1)The high molecular weight component in the raw material is not fully plasticized (2)The barrel temperature is too low and part of the resin is not completely melted (3)The screw mixing effect is insufficient (4)The raw material contains cross-linked or oxidized gel (5)The screen mesh is not enough and the gel is not intercepted
الحل
(1)Appropriately raise the barrel temperature to the higher value within the range of 180-230°C (2)Optimize the screw design and add mixing elements (3)Increase the screen mesh to 80-120 mesh (4)Select high-quality raw materials with low gel content (5)Check whether cross-linked materials are mixed into the regrind
الخلاصة الأساسية
Gel is caused by insufficient plasticization or raw material quality problems, and needs to be solved from temperature control, screw design, and raw material selection.
gelgel particlesplasticization temperaturescrew mixingscreen mesh