Extrusion & Post 13 مشاهدة

Sharkskin on the surface of homopolymer polypropylene extruded products

ظاهرة المشكلة
Periodic rough stripes appear on the extrudate surface, resembling sharkskin, with a rough feel. Sharkskin affects product appearance quality and, in severe cases, mechanical properties; it is common in film and pipe extrusion.
تحليل الأسباب
(1) Extrusion speed too fast; stick-slip alternating flow of the melt occurs at the die exit (2) Die temperature too low; large melt adhesion to the die wall (3) High melt elasticity of homopolymer polypropylene; uneven stress release when exiting the die (4) Insufficient inner wall finish of the die or wear (5) Melt temperature too low; high viscosity makes melt fracture likely
الحل
(1) Appropriately increase die temperature to the higher value within the 200-280°C range (2) Reduce extrusion speed so that the melt die exit speed is below the critical speed (3) Polish die inner wall to Ra≤0.2μm, chrome plating when necessary (4) Increase land length at the die exit to stabilize melt flow (5) Appropriately improve the matching of screw rotation speed and haul-off speed
الخلاصة الأساسية
Sharkskin is the result of stick-slip flow of the melt at the die exit; it is improved by increasing die temperature and reducing extrusion speed.
sharkskinmelt fracturedie temperatureextrusion speeddie polishing