Nozzle drooling in PET '2079851475616104452
ظاهرة المشكلة
Melt drools from the nozzle of the PET '2079851475616104452 machine during mold opening and material charging, affecting the next shot.
تحليل الأسباب
Nozzle temperature is too high and melt viscosity is too low; nozzle hole diameter is on the large side; back pressure is set improperly; PET melt thermal stability is insufficient.
الحل
Reduce nozzle temperature to 260-270°C; use a needle valve shut-off nozzle; reduce nozzle hole diameter; use an anti-drooling program.
الخلاصة الأساسية
PET nozzle drooling affects production stability.