Multi-gate product low weld line strength
ظاهرة المشكلة
Multi-gate PEI products are extremely prone to fracture at the weld line
تحليل الأسباب
PEI molecular chains are rigid with slow diffusion rate, causing insufficient molecular entanglement at the weld surface; the melt temperature has already decreased when converging
الحل
Reduce the number of gates (simplify the flow pattern); increase the melt temperature to 380-390°C to extend the fusion time at the weld surface; use sequential valves to control the opening time of each gate
الخلاصة الأساسية
The rigid molecular chain characteristics of PEI make weld lines particularly weak areas