Molds & Tooling 6 Aufrufe

ABS ejection whitening (stress whitening)

Problembeschreibung
White round spots or radial white marks appear at ejector pin positions, obvious on dark-colored parts, affecting appearance.
Ursachenanalyse
During ejection, the product is locally sheared beyond yield, producing stress whitening; too large ejection force, insufficient product cooling, small draft angle, or small ejector pin area are the inducements, related to ABS's high rigidity and large gripping force.
Lösung
①Extend the cooling time to lower the ejection temperature; ②increase the ejector pin cross-sectional area and the number of ejector pins to disperse the force; ③reduce the holding pressure to reduce the gripping force; ④polish the cavity around the ejector pins; ⑤optimize the ejector pin layout to areas of high rigidity.
Wichtigste Erkenntnis
ABS ejection whitening=an alarm of 'ejection force exceeding the standard': disperse the ejection force, give sufficient cooling, and reduce the gripping force to eliminate it; the ejection whitening position is the ejector pin position, and following it to find the cause is the fastest.
ABS;ejection whitening;stress whitening;ejection force;cooling