Extrusion & Post 2 Aufrufe

LLDPE Blown Film Melt Fracture

Problembeschreibung
The film surface is overall orange-peel-like and thread-like rough, more severe than sharkskin.
Ursachenanalyse
The outlet shear rate far exceeds the critical value, and the melt becomes overall unstable; low die temperature and excessive output are the main causes.
Lösung
① Reduce output/line speed; ② raise the die temperature; ③ enlarge the die lip gap to reduce shear; ④ use PPA; ⑤ check whether there are abrupt changes in the die flow channel.
Wichtigste Erkenntnis
For melt fracture, first reduce shear, then raise temperature.
LLDPE;blown film;melt fracture;die lip gap;shear