Molds & Tooling 2 Aufrufe

PA66 mold temperature 80-120℃

Problembeschreibung
Uneven product crystallization, poor surface gloss, thin-walled parts dimensions drift over time
Ursachenanalyse
When mold temperature is below 40℃, PA66 thin-walled parts' crystallinity changes over time, dimensions become unstable; mold temperature around 80℃ gives uniform crystallization and stable physical properties; high mold temperature also reduces internal stress and improves dimensional stability
Lösung
①Mold temperature conventionally 80℃, 80-120℃ for precision and thick-walled parts; ②thin-walled parts with mold temperature below 40℃ need annealing to stabilize dimensions; ③cavity temperature difference controlled within ±2℃
Wichtigste Erkenntnis
Mold temperature determines PA66 crystallinity and thus physical properties; 80℃ is the baseline, ±2℃ temperature difference control can reduce shrinkage fluctuation by 40%; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
PA66; mold temperature; 80℃; crystallinity; ±2℃