Material Drying 3 Aufrufe

PA6 Drying Temperature 80-100°C

Problembeschreibung
After drying, the pellets turn yellow and oxidize, or with insufficient drying the products still show silver streaks
Ursachenanalyse
Drying temperature below 80°C results in insufficient dehydration efficiency, while above 100°C the PA6 surface oxidizes and discolors; ordinary hot-air drying also brings moisture from humid air back into the pellets, making them wetter the more they are dried
Lösung
①Dehumidifying dryer at 80-100°C for 4-8h; ②for oxidation-sensitive natural-colored material, the drying temperature does not exceed 75°C; ③a dehumidifying dryer with a molecular sieve must be used rather than ordinary hot air
Wichtigste Erkenntnis
The key equipment for PA6 drying is the dehumidifying dryer; hot-air drying may be counterproductive in humid seasons, with the temperature upper limit preventing oxidation and the lower limit ensuring efficiency; after confirming effectiveness, fix the parameters and practices into the work instructions to prevent recurrence
PA6;drying temperature;80-100°C;dehumidifying drying;oxidation