Material Drying 3 Aufrufe

PA6 Flame-Retardant Grade Drying

Problembeschreibung
When flame-retardant PA6 is dried at 100°C, particle agglomeration and color darkening occur
Ursachenanalyse
Some flame retardants (especially bromine-based and nitrogen-based) begin to soften or decompose at around 100°C; excessively high drying temperature causes the particle surface to become sticky and agglomerate, and flame retardant decomposition causes discoloration
Lösung
The drying temperature of flame-retardant PA6 is controlled at 80-90°C according to supplier guidance, for 4-6 hours; when agglomeration occurs, lower the temperature and turn the material layer; when discoloration is severe, stop using that batch of material
Wichtigste Erkenntnis
The drying temperature of flame-retardant grades is limited by the temperature resistance of the flame retardant, and conventional conditions cannot be copied directly; after confirming effectiveness, fix the parameters and practices into the work instructions to prevent recurrence
PA6flame retardantdrying temperatureagglomeration