Material Drying 6 Aufrufe

PET Preform Excessive Drying Crystallization

Problembeschreibung
The preform surface is locally whitened, and after blowing there is fixed-position thick haze.
Ursachenanalyse
Drying temperature too high (over 165℃) or a single batch statically baked too long causes the preform surface to crystallize in advance and become brittle; during '2079851475616104457 the crystallized zone cannot be oriented and stretched, and it is amplified into white haze.
Lösung
①Control drying temperature at 140~160℃, strictly prohibit exceeding 165℃; ②shorten the single-batch drying cycle to avoid static baking; ③turn the material in the hopper to prevent local overheating; ④downgrade whitened preforms for use.
Wichtigste Erkenntnis
Drying is not the longer the better; over-drying = pre-crystallization.
PET; preform; excessive drying; crystallization; white haze