PP Injection Part Sink Mark—Freeze-off Type

Problembeschreibung
Although the gate is small and holding time is already long, thick walls still have sink marks.
Ursachenanalyse
The small gate freezes off early, and holding pressure cannot continue to transmit to thick-wall areas; no matter how long the holding time, it is ineffective.
Lösung
①Enlarge the gate to delay freeze-off; ②place the gate near thick-wall areas; ③reduce material at thick walls; ④auxiliary gates if necessary.
Wichtigste Erkenntnis
Holding after freeze-off = ineffective feeding—the gate is the key.
PP;sink mark;gate freeze-off;holding pressure;thick wall