Molds & Tooling 3 Aufrufe

PPO burnt marks

Problembeschreibung
Burnt marks and brown streaks appear at fixed positions of PPO products, mostly at flow ends and material convergence areas; they improve briefly after machine purging and then recur.
Ursachenanalyse
When mold venting is poor, the compressed air heats up adiabatically and burns the melt; stagnant material dead spots in the barrel and nozzle decompose under long-term heating and are carried into the product; excessive melt temperature aggravates the heat damage risk.
Lösung
①For fixed-position burning, prioritize checking venting and adding vent grooves; ②clean the stagnant material dead spots of the barrel and nozzle; ③appropriately reduce the melt and mold temperatures; ④adjust the filling rate to prevent trapped gas.
Wichtigste Erkenntnis
For PPO burning, first distinguish the two causes of venting trapped gas and equipment stagnant material; fixed positions are characteristic of venting problems; random distribution points to equipment dead spots.; after confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence
PPO; burning; venting; stagnant material; dead spots; trapped gas