Extrusion & Post 9 Aufrufe

EMA Extruded Film Has Transverse Ripples

Problembeschreibung
Transverse periodic ripples with wavelength 5-10mm on the surface of EMA extruded film
Ursachenanalyse
Haul-off roller vibration or unstable speed produces periodic stretching changes; cooling roller eccentric or out-of-round surface causes periodic contact pressure changes
Lösung
1) Overhaul the haul-off roller to eliminate vibration; 2) Round-calibrate the cooling roller, eccentricity <0.02mm; 3) Install a pressure stabilizing device on the extruder to eliminate pressure fluctuation; 4) Stably control haul-off speed within ±0.5%
Wichtigste Erkenntnis
Transverse ripples are caused by haul-off vibration and roller eccentricity; equipment overhaul and stable control are key
EMA film transverse ripples haul-off vibration cooling roller eccentricity pressure stabilizing device