Extrusion & Post 9 Aufrufe

Excessive thermal shrinkage of EVA film

Problembeschreibung
EVA film thermal shrinkage at 80°C >12%, exceeding the 5% dimensional stability requirement
Ursachenanalyse
EVA extrusion orientation releases upon heating causing large shrinkage; EVA thermal expansion coefficient large; film cooling froze large amount of orientation stress
Lösung
1) Reduce extrusion draw ratio to reduce orientation freezing; 2) Film annealing treatment at 60-80°C to release orientation stress; 3) Add 5-10wt% rigid resin to reduce thermal shrinkage; 4) Biaxial stretching process to balance orientation
Wichtigste Erkenntnis
Film thermal shrinkage is caused by orientation freezing; reducing draw ratio and annealing treatment are key
EVA film thermal shrinkage orientation release annealing treatment biaxial stretching

War das hilfreich?