Injection Molding 4 Aufrufe

Flow marks in EVA '2079851475616104452

Problembeschreibung
Radial flow marks centered on the gate appear on EVA injection molded product surface
Ursachenanalyse
Injection speed too fast causing unstable melt front; mold temperature too low <30°C with front cooling rapidly forming marks
Lösung
1) Adopt multi-stage injection speed slow-fast-slow to control front stability; 2) Increase mold temperature to 40-50°C to delay front cooling; 3) Stabilize injection pressure to avoid fluctuation; 4) Enlarge gate area to reduce pressure abrupt change at gate
Wichtigste Erkenntnis
Flow marks are caused by unstable injection front and rapid cooling; multi-stage injection and high mold temperature are key
EVA injection flow marks injection speed mold temperature gate area