Flow marks in EVA '2079851475616104452
Fenómeno do problema
Radial flow marks centered on the gate appear on EVA injection molded product surface
Análise das causas
Injection speed too fast causing unstable melt front; mold temperature too low <30°C with front cooling rapidly forming marks
Solução
1) Adopt multi-stage injection speed slow-fast-slow to control front stability; 2) Increase mold temperature to 40-50°C to delay front cooling; 3) Stabilize injection pressure to avoid fluctuation; 4) Enlarge gate area to reduce pressure abrupt change at gate
Conclusão principal
Flow marks are caused by unstable injection front and rapid cooling; multi-stage injection and high mold temperature are key