Molds & Tooling 3 Aufrufe

EVOH Internal Shrinkage Cavities

Problembeschreibung
Shrinkage cavities 0.5-2mm in diameter at the center of EVOH thick-walled products
Ursachenanalyse
After cooling of the thick-walled area, the interior shrinks but the surface is already solidified and cannot be fed; holding time insufficient, gate freezes too early
Lösung
1) Extend holding time until the gate fully freezes; 2) Increase gate size to delay freezing; 3) Product design to reduce wall thickness differences
Wichtigste Erkenntnis
Shrinkage cavities are caused by thick-wall shrinkage and insufficient holding; extending holding is key