Extrusion & Post 9 Aufrufe

Transverse Ripples on CMC Extruded Film

Problembeschreibung
Transverse periodic ripples with wavelength 5-10mm on the surface of CMC extruded film
Ursachenanalyse
Haul-off roller vibration or unstable speed produces periodic stretching changes; cooling roller eccentricity or out-of-round surface causes periodic contact pressure changes
Lösung
1)Overhaul haul-off rollers to eliminate vibration; 2)Round cooling rollers with eccentricity <0.02mm; 3)Install pressure stabilizing device on the extruder to eliminate pressure fluctuations; 4)Stable control of haul-off speed ±0.5%
Wichtigste Erkenntnis
Transverse ripples are caused by haul-off vibration and roller eccentricity; equipment overhaul and stable control are the key
CMC filmtransverse rippleshaul-off vibrationcooling roller eccentricitypressure stabilizing device