POE surface stress whitening
Problembeschreibung
POE product stressed area surface stress whitening, affecting appearance and strength
Ursachenanalyse
POE under local stress, molecular orientation causes refractive index difference and whitening; product internal stress concentration areas
Lösung
1) Reduce injection speed to reduce orientation stress; 2) Annealing treatment 80°C/2h to release stress; 3) Product design to avoid stress concentration sharp corners
Wichtigste Erkenntnis
Stress whitening is caused by orientation and internal stress; reducing orientation and annealing are key