Extrusion & Post
3 Aufrufe
Metallocene linear low density polyethylene blown film wrinkles(Variant: Strengthened Measures)
Problembeschreibung
Longitudinal wrinkles appear in the film during hauling, affecting film flatness and subsequent processing.
The wrinkles become more obvious after winding, and in severe cases cause the film to be scrapped.In particular, extra attention is needed on top of the original basis, this problem is more prominent and requires key attention.
Ursachenanalyse
(1) Film thickness uneven, thin parts shrink first producing wrinkles\
(2) Haul-off roll pressure uneven\
(3) Collapsing frame angle improper or the included angle asymmetric\
(4) Cooling line height unstable\
(5) Uneven cooling at various parts of the film causes different shrinkage\
(6) On top of the original basis, extra attention is needed: process parameter fluctuations or equipment status changes aggravate this problem
Lösung
(1) Adjust the die gap and air ring, ensure uniform film thickness\
(2) Adjust the haul-off roll pressure, ensure uniform clamping\
(3) Adjust the collapsing frame angle symmetrically, generally an included angle of 30-45°\
(4) Stabilize the cooling line height, fluctuation not exceeding ±50mm\
(5) Check the air ring cooling uniformity, replace with a high-efficiency air ring if necessary\
(6) And strengthen process monitoring; on top of the original basis, extra attention is needed, paying special attention to parameter stability
Wichtigste Erkenntnis
Wrinkles are caused by uneven thickness or unbalanced hauling, and need to be solved from thickness control, hauling and collapsing frame adjustment.Targeted preventive measures need to be taken in different production scenarios.