Problembeschreibung
Bubbles and silver streaks appear inside or on the surface of PAR transparent products.
Ursachenanalyse
PAR has high heat resistance and strong moisture absorption; when the moisture is >0.02%, the moisture vaporizes during high-temperature processing, producing bubbles and silver streaks.
Lösung
Dry at 120-140°C for 4-6h to moisture <0.02%; use a dehumidifying dryer with a dew point ≤-35°C.
Wichtigste Erkenntnis
Strict PAR drying requirements are the prerequisite for high transparency.