Molds & Tooling 3 Aufrufe

PAEK insufficient crystallinity, low performance

Problembeschreibung
The product has insufficient crystallinity, appearing translucent, with poor mechanical properties
Ursachenanalyse
Mold temperature <160°C causes quenching forming amorphous structure; cooling speed too fast and molecular chains have no time to arrange
Lösung
Increase the mold temperature to 180-200°C; post-process at 200°C/2h to promote crystallization
Wichtigste Erkenntnis
PAEK crystallinity is the most important performance control indicator
crystallinityamorphousmold temperaturepost-processing