Injection Molding 6 visualizaciones

ASA chevron surface defect

Fenómeno del problema
ASA weather-resistant product surface shows chevron (chevrons) patterns, accompanied by uneven haze and step-shaped defects, positions related to the flow front.
Análisis de la causa
Academic research confirms that ASA '2079851475616104452 surface defects originate from flow instability: recoverable shear strain, shear stress and mold wall friction coefficient are the key control factors; melt slip instability forms the characteristic pattern.
Solución
①Reduce injection speed to reduce shear stress and recoverable strain; ②raise mold temperature to reduce melt-mold wall friction difference; ③optimize gate to avoid high-speed direct impact; ④adjust material grade viscosity if necessary.
Conclusión clave
ASA chevron defect is a rheological instability problem rather than a conventional process defect; the three elements of shear strain, stress, and friction are the governance direction; academic mechanism guides parameter adjustment more efficiently.
ASA; chevron; flow instability; shear stress; haze; friction