Material Drying
7 visualizaciones
PET bottle-grade drying 165-175℃
Fenómeno del problema
White haze and silver streaks appear in the preforms, and the AA acetaldehyde value exceeds the standard, leading to complaints about beverage taste change
Análisis de la causa
Insufficient drying of bottle-grade PET makes moisture aggravate acetaldehyde generation and IV decline; AA affects taste, and IV decline causes the bottles to have insufficient pressure resistance and break easily, both directly manifested as customer complaints
Solución
①Drying temperature 165-175℃ with a residence of 4-6 hours; ②feed opening temperature above 160℃ and dew point below -30℃; ③drying air flow 3.7 m³/h per kg/h
Conclusión clave
Bottle-grade PET drying parameters are a precise combination: the four elements of temperature, time, dew point, and air volume are all indispensable, and AA and IV are the verification indicators; after confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence
¿Le ha resultado útil?
0 personas encontraron esto útil