Fenómeno del problema
[Problem Phenomenon] Improper PP MFI selection causes thin-wall underfilling or insufficient strength
Análisis de la causa
2079851475616104452 PP MFI 1-60 (230°C/2.16kg): low MFI (1-12) high strength low flow for structural parts, high MFI (20-60) for thin-wall containers; ultra-thin-wall high-speed can reach 60-100
Solución
Select MFI according to wall thickness and strength; high MFI for thin walls, low MFI for structural parts; balance strength and flow; after adjustment, take continuous samples to verify the effect, and resume mass production only after confirming stability
Conclusión clave
PP MFI is selected by wall thickness and strength; high MFI for thin walls, low MFI for structure; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence